1.Measurement on a flat board by a tribometer (Fukushima Prefecture High Tech Plaza)
TRIBOMETER made by Nanometric Technology Inc.

Load |
:1N |
Friction radius |
:5mm |
Rotation speed |
:1rpm(0.05cm/sec) |
Ball |
:SUJ2 make 6mmφsteel ball |
n=3 |
Zero Chromium S |
hexavalent chromate |
friction coefficient |
0.409 |
0.547 |
2.Measurement on a flat board by a tribogear (Tochigi Prefecture Industrial Technology Center)
Tribogear made by SHINTO scientific Co., Ltd.

Friction |
:10mmφ SUS304 |
Added load |
:50gf |
Friction speed |
:10mm/sec |
Measurement length |
:20mm |
n=2 |
Zero Chromium S |
hexavalent chromate |
friction coefficient |
0.451 |
0.376 |
3.Measurement by a screw fastener testing machine (Osaka Prefecture Industrial Technology General Research Center)
Screw fastener testing machine

M |
:10×60 |
Pace |
:1.5 |
Circular seating surface |
:outer diameter 16.5
inner diameter 11.5 |
n=5 |
Zero Chromium S |
hexavalent chromate |
Zero Chromium SB |
hexavalent black |
coefficient |
0.300 |
0.304 |
0.366 |
0.256 |
torque pressure(N・m) |
27.3 |
27.6 |
33.0 |
23.6 |